The clinical success of orthodontic treatment hinges on the durability of bracket adhesion to enamel, which is influenced by the choice of bonding agent. This study aimed to evaluate and compare the shear bond strength and adhesive remnant index (ARI) of four contemporary orthodontic bonding systems: a self-etching primer system (Transbond Plus Self-Etching Primer), a light-cure composite adhesive (Ultimate cure-on-light), a self-cure composite (Ortho-one no-mix), and a light-cure glass ionomer cement (G.C. Fuji Ortho L.C.). The investigation focused not only on bond strength but also on the amount of adhesive residue left on the enamel surface after debonding, which is critical for minimizing iatrogenic enamel damage.
Forty-eight extracted human premolars were selected based on strict inclusion criteria: intact buccal surfaces, absence of caries or cracks, and no prior chemical treatment. Teeth were cleaned, stored in distilled water, and polished with non-fluoridated pumice before use. Eighty pre-adjusted edgewise brackets (0.022″ slot, American Orthodontics) were randomly assigned to four groups of 20 brackets each.Zinc Protoporphyrin NF-κB Group I used Ultimate cure-on-light (light-cure composite), Group II used Ortho-one no-mix (self-cure composite), Group III used G.Spartalizumab In Vitro C. Fuji Ortho L.C. (light-cure glass ionomer), and Group IV used Transbond Plus Self-Etching Primer (acidic primer + light-cure composite).PMID:34549837 Enamel conditioning protocols were applied accordingly: 37% phosphoric acid for Groups I and II (60 seconds), 20% polyacrylic acid for Group III (20 seconds), and direct application of the self-etching primer for Group IV (5 seconds, no rinsing).
All brackets were bonded following standardized procedures. Excess adhesive was removed with a scaler, and curing was performed using a halogen light unit (20 seconds per surface). Samples were stored in distilled water at 37°C for 24 hours prior to testing. Shear bond strength was measured using a Hounsfield Universal Testing Machine at a crosshead speed of 1 mm/min. The peak force required to debond each bracket was recorded and converted into MPa. After failure, teeth were examined under a stereomicroscope (10x magnification) to assess residual adhesive using the ARI scale (1 = all adhesive remains; 5 = no adhesive remains).
Statistical analysis revealed significant differences among groups (P < 0.01). Group IV (Transbond Plus Self-Etching Primer) demonstrated the highest mean shear bond strength (8.69 ± 1.78 MPa), followed by Group I (8.62 ± 1.84 MPa), Group II (8.07 ± 1.72 MPa), and Group III (6.01 ± 1.69 MPa). ARI scores showed that Group III had the highest average score (3.4), indicating substantial adhesive retention, while Group IV had the lowest (2.1), suggesting minimal residue. Group I and II showed intermediate ARI values (2.8 and 2.6, respectively). These findings indicate that self-etching primers provide superior bond strength and reduce adhesive remnants, which may lower the risk of enamel demineralization and microfractures during debonding. While light-cure composites offer high bond strength and predictable performance, self-cure systems require longer setting times and are more technique-sensitive. Light-cure glass ionomer cements, though beneficial for fluoride release and enamel preservation, exhibited the weakest bond strength in this study. In conclusion, the use of self-etching primer systems offers a clinically advantageous balance between high shear bond strength, reduced chairside time, and favorable adhesive remnant patterns. These results support their preference in modern orthodontic practice, especially when bonding ceramic brackets where enamel integrity is paramount. Future research should explore long-term stability and performance under varying oral conditions.MedChemExpress (MCE) offers a wide range of high-quality research chemicals and biochemicals (novel life-science reagents, reference compounds and natural compounds) for scientific use. We have professionally experienced and friendly staff to meet your needs. We are a competent and trustworthy partner for your research and scientific projects.Related websites: https://www.medchemexpress.com